Brazing is a long-established and widely used metal-joining method. It involves joining metals using a filler material with a melting point above 450 °C, while keeping the base metals below their melting points. This study aims to investigate the effect of joint gap widths specifically 0.10 mm and 0.30 mm on the tensile strength of ST40 steel joints brazed with CuZn40 brass; to determine the optimal joint gap width for achieving maximum tensile strength; and to identify the failure modes and joint efficiency of the ST40 steel–CuZn40 brass joints in terms of tensile strength. The results indicate that varying the joint gap width between 0.10 mm and 0.30 mm does not significantly affect the optimal tensile strength. A gap width of 0.30 mm yielded a higher average tensile strength (333.23 MPa) compared to a gap width of 0.10 mm (283.09 MPa). All specimens failed at the joint, exhibiting a brittle failure pattern (with Fp/Fm ratio ranging from 0.539 to 0.997).